    Buildings & Facilities · Chapter 36Applied

    By Kurnia · Published November 13, 2026 · Version 1 · 20 min read

    Cracks in walls and concrete

    types and causes of cracks, structural and nonstructural cracks, measuring and monitoring crack width, seepage and dampness, plaster repair, and when to call a structural engineer

    A diagonal crack appears from the corner of a door frame in a corridor near a hospital laundry, the door starts to stick, and the technician is about to cover it with skim coat and paint. This chapter covers cracks in plastered brick walls and concrete from the building technician’s side: causes of cracking such as shrinkage, temperature, moisture, ground settlement, load, and reinforcement corrosion, the difference between cracks suspected to be structural and those that are not, how to measure crack width and monitor its change, seepage and damp walls, plaster and mortar joint repair for nonstructural cracks, and the signs that require a structural engineer to be called. American building preservation guidance and a building damage category table from a British government document are used as data from their countries of origin. The chapter gives no method for judging structural strength; cracks suspected to be structural are always handed to a structural engineer.

    Section you’re reading: Chapter opening

    In a service corridor of a hospital, between the laundry room and the linen store, the cleaning staff report a crack that runs diagonally from the top corner of a door frame toward the ceiling. The same door has started to stick at the top, and on the outside face of that wall the plaster near the floor is bulging with patches of white salt. The duty technician has already prepared skim coat and paint so the corridor looks tidy before the accreditation visit. The supervisor asks for one thing first: the ends of the crack are marked and dated, its width is measured, and the door is noted. Two weeks later the crack has grown past its end marks and its width has increased.

    A skim coat patch would cover the only sign that the wall is still moving. A crack is a record of movement, and its value to an inspection depends on leaving it readable until someone with authority has assessed it. The building technician does not decide whether a wall or beam is still strong; the technician’s work is to recognize crack patterns, measure and monitor their change, find the source of the water that comes with them, repair the cracks that really are cosmetic, and know when to stop.

    Scope

    This chapter covers cracks in plastered brick walls, plaster, and concrete in buildings from the building technician’s side: causes and patterns of cracking, telling cracks suspected to be structural from those that are not as a basis for reporting, measuring and monitoring crack width, seepage and damp walls, plaster and mortar joint repair for nonstructural cracks, and when a structural engineer is called. This chapter gives no method for judging structural strength. Cracks suspected to be structural are always handed to a structural engineer, an engineer authorized to assess structures and design structural repairs.

    Loads, structural elements, and load paths are in Chapter 1; mold on damp walls in Chapter 9 · Biology & Microbiology; reinforcement corrosion from the chemical side in Chapter 19 · Chemistry on electrochemical corrosion; water entering through the roof in Chapter 35 on roofs and waterproofing; paints and coatings in Chapter 37 on building paints and coatings; and work on high facades in Chapter 10 · Safety on work at height. The status and content of the building maintenance and upkeep guidelines of the Ministry of Public Works and Housing (Permen PU 24/PRT/M/2008) and of PP 16/2021 cannot yet be confirmed as of November 2026; check with JDIH PUPR before using them for schedules or audits.

    Work outside the building technician’s authority: judging the strength of walls, beams, columns, or slabs; injecting resin to restore the strength of a crack; chiseling concrete down to the reinforcement, cutting reinforcement, or installing props; demolishing walls; and scraping old plaster or paint that may contain lead or asbestos. That work belongs to a structural engineer, an appointed contractor, or a contractor authorized for hazardous materials.

    Why walls and concrete crack

    Concrete, brick, mortar, and plaster are strong in compression but weak in tension. When part of a building is forced to lengthen, shorten, or deflect more than its tensile strength can bear, the material releases the stress by cracking. A crack pattern therefore carries clues about the movement that caused it. American concrete preservation guidance notes that cracking occurs in most concrete and varies in depth, width, direction, pattern, and location.

    The causes building technicians meet most often:

    1. Early shrinkage. Concrete and plaster shrink as they dry. Fine random cracks that resemble the lines on a map, called map cracking, usually come from early shrinkage, but they can also indicate other deterioration such as alkali-silica reaction. In plaster, map cracking appears when the finish coat is applied over a base coat that has too much sand or is too thin.
    2. Thermal movement. Concrete expands and contracts with temperature. Thermal cracks often appear at the ends or re-entrant corners of older concrete buildings built without expansion joints.
    3. Moisture movement. Porous materials swell when wet and shrink when dry; cracks that open and close with the seasons belong to this type.
    4. Ground settlement and vibration. Diagonal cracks running in opposite directions point to building settlement and soil conditions; clay soil swells in the rainy season and shrinks in the dry season, and vibration from heavy traffic or blasting gives similar symptoms.
    5. Overloading. Stresses within a wall can produce diagonal cracks that usually start at a door or window frame, including where a new opening was made without a beam above it.
    6. Reinforcement corrosion. Rust on reinforcing steel expands and pushes the concrete cover until it cracks and spalls; spalling can reduce the structure’s ability to carry loads.

    The size of thermal movement can be estimated with

    ΔL=α L ΔT\Delta L = \alpha \, L \, \Delta T

    where ΔL\Delta L is the change in length (m), α\alpha the coefficient of linear expansion of the material (per kelvin), LL the length of the part that is free to move (m), and ΔT\Delta T the change in temperature (K). The formula assumes the part is free to expand; a wall or slab restrained at its ends does not move that freely, so the restrained movement turns into stress and cracking (Example 1). The value of α\alpha is taken from data for the material used.

    Structural and nonstructural cracks

    A structural crack is a crack caused by forces on the structure. The American concrete guidance names its causes: temporary or continued overloads, uneven foundation settling, seismic forces, or original design inadequacies. An active crack is a crack that is still widening, deepening, or lengthening; a dormant crack is a crack whose size stays relatively unchanged. A structural crack is active if an overload or settlement is continuing, and becomes dormant once the load has been removed or the settlement has stabilized. Dormant early shrinkage cracks are generally not a structural concern, but they still become a path for water if left alone.

    The technician does not decide whether a crack is structural. What the technician can do is recognize the signs that make a crack suspected to be structural, and therefore reported to a structural engineer: cracks in beams, columns, slabs, or load-bearing walls; diagonal or stepped cracks that pass through a wall, especially from the corner of an opening; cracks that widen from one measurement to the next; doors and windows that start to stick; walls that lean or bulge; floors or beams that sag; and spalled concrete exposing rusted reinforcement. The American plaster guidance gives an equally simple example: a dark crack at the junction of two walls may be a structural crack and should be investigated for its underlying cause.

    Structural engineers and building surveyors use damage scales to record the condition of brick buildings. The ground settlement policy paper of a British high-speed rail project contains a scale based on the work of Burland and colleagues (1977):

    CategoryDegree of damageTypical damage in brick buildingsApproximate crack width (mm)
    0Negligiblehairline cracksnot given
    1Very slightfine cracks easily treated during normal redecoration0.1 to 1
    2Slightcracks easily filled, redecoration needed, doors and windows may stick slightly1 to 5
    3Moderatecracks may need cutting out and patching, doors and windows stick, weathertightness often impaired5 to 15, or several cracks above 3
    4Severeextensive repair removing parts of walls, frames distorted, floors slope, walls lean or bulge15 to 25, depending on the number of cracks
    5Very severemajor repair up to rebuilding, beams lose bearing, danger of instabilityusually above 25, depending on the number of cracks

    The same document gives a note that governs how the table is read: crack width is only one aspect of damage and should not be used on its own as a direct measure of it. The table is British data for brick buildings. For the building technician, it is useful as reporting vocabulary, for example “3 mm crack with a sticking door”, while assigning the category and the cause remains the work of a structural engineer.

    Measuring and monitoring crack width

    Measuring a crack answers two questions: how wide it is, and whether it is changing. The second question matters more. The American concrete guidance acknowledges that it is difficult to determine whether cracks are moving, so most cracks are assumed to be moving. For that reason, monitoring starts before any repair.

    Common tools and methods:

    1. A crack width gauge card, a card with lines of known width that are matched against the crack width; quick, and sufficient for hairline cracks up to a few millimeters.
    2. End marks and dates. The ends of the crack are marked with a pencil line at right angles, with the date, so any lengthening shows at the next inspection.
    3. Gauge studs, two small pins or bolts set on either side of the crack; their distance is measured with calipers, and a change in distance shows the crack opening (Example 5).
    4. A grid crack monitor, two overlapping plates fixed across the crack, one with crosshairs and one with a grid, so horizontal and vertical movement can be read separately (Example 4).
    5. Scaled photographs from the same position and distance, with a ruler beside the crack.

    Every reading is recorded with the date, time, air temperature, and weather, because cracks caused by temperature or moisture open and close with the seasons. The rate of change is calculated as

    r=w2−w1t2−t1r = \frac{w_2 - w_1}{t_2 - t_1}

    where rr is the rate of widening (mm per month), w1w_1 and w2w_2 the crack width (mm) at the first and second measurements, and t2−t1t_2 - t_1 the interval between them (months). A change smaller than the resolution of the measuring tool does not prove that the crack is moving, nor does it prove that the crack is still. The American moisture guidance notes that diagnosing complicated problems can take several months up to four seasons of monitoring, and monitoring building cracks needs the same patience. A sequential record with photographs and notes on changes in size, related to temperature and rainfall, is the material a structural engineer reads.

    Seepage and dampness

    Cracks and water make each other worse. A crack opens a path for rainwater, and water carries salts, dissolves mortar, swells materials, and speeds up reinforcement corrosion. The American moisture guidance names the five most common sources of water: exterior water above ground level, ground water below ground level, leaking pipes and mechanical equipment, moisture from room use and air-conditioning systems, and water from maintenance work and building materials. Rainwater from the roof or overflowing gutters, leaking pipes, and splash-back from hard paving beside a wall are among the sources that wet walls and damage the plaster on their inner face.

    Plaster on a brick wall that is always wet is easily damaged: salts from the wall are carried to the surface and appear as dry bubbles or efflorescence, a white salt deposit on the surface, and the source of the water must be eliminated before the plaster is repaired. The same guidance warns that repairs over a wet base will fail again, so plaster damaged by water from the ground sometimes has to be removed so the wall can dry out.

    Two simple checks help tell water coming from the wall from water coming from the air. First, a resistance-type moisture meter can show whether a wall surface is drying out or getting damper over time. Second, a sheet of foil is taped to the surface of a brick wall and checked after a day or two: if water forms behind the foil, it comes from the wall; if water is on the surface of the foil, it comes from condensing air. Condensation and the mold that comes with it are covered in Chapter 9 · Biology & Microbiology. A waterproof coating on the wall surface does not replace cutting off the water source, because an impermeable layer can hold water inside the material.

    Plaster repair and nonstructural cracks

    Repair starts with the cause. American mortar joint guidance stresses that the cause of deterioration, such as a leaking roof or gutter, uneven settlement of the building, capillary rising damp, or extreme weather exposure, must be dealt with before repair work begins; without that, the deterioration continues and the repair is wasted. For cracks caused by structural movement, the structure is repaired first according to the structural engineer’s design, and only then the plaster.

    For cracks that really are cosmetic, the American plaster guidance gives a graded sequence. Hairline cracks in sound plaster are no cause for concern and can be filled with patching material. Cracks that reopen with seasonal changes in humidity are widened slightly with a pointed tool and then filled. Cracks that keep coming back are bridged with fiberglass mesh tape pressed into the patching material, covered with a second coat, then a third coat to level the surface before light sanding. The same guidance closes this part with a sentence this chapter uses as its rule: if a crack seems to be widening, a structural engineer should be consulted.

    In brick and stone walls, cracks often follow the mortar joints. Replacement mortar must be softer and more vapor-permeable than the brick or stone, and no harder than the old mortar; mortar stronger than its bricks leaves no room for movement, so the stress is released through the bricks and causes cracking and spalling that are hard to repair. In concrete, hairline cracks that show no sign of growing can often be left unrepaired, non-moving cracks can be filled with a matching cement mortar, and active cracks are filled with a flexible sealant that bonds to both sides of the crack after a groove has been cut and cleaned. Epoxy injection to restore the structural integrity of dormant cracks is a decision and a job under a structural engineer.

    Scraping and removing old plaster creates dust. The American plaster guidance asks demolition workers to wear masks approved by the American occupational safety agency, long-sleeved clothing, and head and eye protection, because the dust can contain soot, lead from old paint, or asbestos. PPE is covered in Chapter 5 · Safety, and old paint in Chapter 37 on building paints and coatings.

    When to call a structural engineer

    A structural engineer is called when there are signs that a crack comes from forces on the structure or when a crack is changing, not when a patch fails for the second time. A good technician’s report speeds up that assessment. It contains: the crack location measured from a recognizable column line or wall as in Chapter 1 on loads and load paths; the element that is cracked; direction and pattern; length and width with the measuring tool used; the history of readings and their dates; scaled photographs; other symptoms such as sticking doors, sloping floors, seepage, or sounds; and preceding events, such as an earthquake, renovation, wall removal, new heavy machinery on the floor above, a long-running pipe leak, or a large tree near the foundation.

    Until the structural engineer arrives, the crack is not patched and not painted, because a patch erases the end marks and width that are the evidence of movement. There is no load test or stepping test to “prove” that a wall or floor is still strong, and no improvised emergency props. Where there are signs of immediate danger, such as falling material, a bulging wall, or a crack opening quickly, the area is cordoned off and cleared according to the building’s emergency procedure.

    Worked example

    The numbers in the examples below are practice numbers, unless their origin is stated.

    Example 1: thermal movement of a long concrete wall. A 20 m concrete boundary wall without expansion joints undergoes a temperature change of 25 K between a rainy-season night and a hot afternoon. With α=10×10−6\alpha = 10 \times 10^{-6} per K, its free change in length is ΔL=10×10−6×20×25=0.005\Delta L = 10 \times 10^{-6} \times 20 \times 25 = 0.005 m, that is 5 mm. If both ends are restrained, that 5 mm movement does not happen and turns into stress, so a crack appears at the weakest point. A crack that opens and closes with temperature like this is filled with a flexible sealant, not rigid mortar.

    Example 2: crack width and the British damage categories. A 0.4 mm crack in the plaster of a room wall with no other symptoms falls in the range 0.1 to 1 mm, matching the description of category 1 in the British table. A 6 mm diagonal crack from the corner of a door frame with a sticking door falls in the range 5 to 15 mm, and its description matches category 3. The technician records the width and symptoms without assigning a category; the second crack is suspected to be structural because of its pattern and symptoms, so it is reported to a structural engineer, while the first is monitored and may be repaired as a cosmetic crack if it does not change.

    Example 3: rate of widening. Gauge card readings in the opening case: March 1, 0.30 mm; April 1, 0.35 mm; May 1, 0.45 mm; June 1, 0.60 mm. In three months the width grew by 0.60−0.30=0.300.60 - 0.30 = 0.30 mm, so r=0.30/3=0.10r = 0.30/3 = 0.10 mm per month. The monthly increases were 0.050.05, 0.100.10, and 0.150.15 mm, so the rate is rising. A crack that widens faster and faster is an active crack and meets Stop condition 1.

    Example 4: reading a grid crack monitor. When installed, the crosshairs are at zero. Six weeks later the crosshairs have moved 1.2 mm horizontally and 0.5 mm vertically. The total displacement is 1.22+0.52=1.3\sqrt{1.2^2 + 0.5^2} = 1.3 mm. Vertical displacement means the two sides of the crack are also shifting up and down, not just opening, and that observation is recorded as it is for the structural engineer.

    Example 5: gauge studs and tool resolution. The distance between two gauge studs is 100.42 mm at installation and 100.78 mm three months later, measured with calipers with a resolution of 0.02 mm. The crack opening is 100.78−100.42=0.36100.78 - 100.42 = 0.36 mm, that is 0.36/0.02=180.36/0.02 = 18 times the tool resolution, so the change is real and not a reading error. The next reading uses the same calipers and is taken at the same time of day.

    Example 6: plaster patching material. A cosmetic crack 2.4 m long that has not changed during monitoring is repaired by removing damaged plaster 150 mm wide on each side of the crack and 15 mm thick. The removed area is 2.4×0.30=0.722.4 \times 0.30 = 0.72 m², the material volume 0.72×0.015=0.01080.72 \times 0.015 = 0.0108 m³ or 10.8 L, and with a 10 percent allowance 10.8×1.1=11.910.8 \times 1.1 = 11.9 L. The type of patching material follows the old plaster and the brick wall behind it.

    Stop conditions

    1. The crack is in a beam, column, slab, or load-bearing wall, has a diagonal or stepped pattern passing through the wall, or widens or lengthens between two measurements: do not patch or paint it; continue monitoring and report to the building manager, who calls a structural engineer.
    2. Material is falling, spalled concrete exposes rusted reinforcement, or a plaster ceiling is sagging or coming loose: cordon off and clear the area below without approaching the hazard, then report to the building manager and a structural engineer.
    3. A wall appears to lean or bulge, doors and windows suddenly stick, a floor appears to slope, or cracking sounds are heard: stop using that area and follow the building’s emergency procedure; a structural engineer assesses it before the area is used again.
    4. A new crack appears after an earthquake, vehicle impact, fire, renovation, wall removal, or the addition of a heavy load: the crack is not treated as cosmetic; a structural engineer inspects it before any repair.
    5. The repair would require chiseling concrete down to the reinforcement, cutting reinforcement, injecting resin into the crack, installing props, or demolishing a wall: stop; the work is designed by a structural engineer and carried out by an appointed contractor.
    6. Old plaster or paint that would be scraped or removed may contain lead or asbestos: stop; the material is tested and the work is handed to a contractor authorized to handle it.
    7. A crack or seepage on a facade can only be reached from height: do not use a ladder or makeshift footing; access is chosen and permitted under Chapter 10 · Safety on work at height.
    8. Seepage or a wet wall is near an outlet, panel, or cable: keep people away and ask an authorized electrician to inspect and isolate the circuit.

    Common misinterpretations

    Guess what’s wrong first, then open the explanation.

    Common misconception

    A hairline crack is always harmless.

    Why is it wrong?

    A hairline crack in sound plaster is generally cosmetic, but its location and its change decide. A hairline crack in a beam or column, or a hairline crack that keeps lengthening, is reported like any other crack suspected to be structural.

    Common misconception

    Crack width decides whether a crack is structural.

    Why is it wrong?

    Crack width is only one aspect of damage and is not used on its own as a direct measure. Pattern, the cracked element, other symptoms, and change over time matter just as much.

    Common misconception

    A crack that was patched and has not come back means the problem is solved.

    Why is it wrong?

    A patch can hide movement that is still going on. Cracks are monitored and recorded before they are repaired, and if the cause is structural movement, the structure is repaired first.

    Common misconception

    Harder mortar lasts longer.

    Why is it wrong?

    Mortar stronger than the bricks makes the stress release through the bricks, so the bricks crack and spall. Replacement mortar is softer and more vapor-permeable than its bricks.

    Common misconception

    A damp wall only needs waterproof paint.

    Why is it wrong?

    An impermeable coating can hold water inside the wall and speed up the damage. The water source is found and stopped first, and only then are the plaster and paint repaired.

    Chapter 1 on loads, structural elements, and load paths explains why the location of a crack relative to the supports matters and why its assessment belongs to a structural engineer. Chapter 19 · Chemistry on electrochemical corrosion explains the reinforcement corrosion that spalls concrete, Chapter 9 · Biology & Microbiology covers mold on damp walls, and Chapter 35 on roofs and waterproofing covers water coming from above. Wall paints and coatings are covered in Chapter 37 on building paints and coatings, PPE for demolition dust in Chapter 5 · Safety, and access to high facades in Chapter 10 · Safety on work at height.

    Exercises and worked solutions

    The numbers in the exercises are for practice.

    Try to answer first, then open the worked solution.

    1. A 30 m concrete wall without expansion joints undergoes a temperature change of 20 K. With α=10×10−6\alpha = 10 \times 10^{-6} per K, what is its free change in length, and what does it mean for cracks at its ends?

      Check my answer
      See the worked solution

      ΔL=10×10−6×30×20=0.006\Delta L = 10 \times 10^{-6} \times 30 \times 20 = 0.006 m, that is 6 mm. If the ends of the wall are restrained, that movement becomes stress that can crack the ends or corners, so cracks that open and close with temperature are filled with a flexible material and expansion joints are discussed with a structural engineer.

    2. A plaster crack reads 0.20 mm in January and 0.22 mm in July on a gauge card with a resolution of 0.05 mm. Is the crack proven to be moving or proven to be still?

      Check my answer
      See the worked solution

      Neither. The change of 0.02 mm is smaller than the 0.05 mm resolution, so the reading neither proves movement nor proves the crack is still; monitoring continues, preferably with a more precise tool such as gauge studs and calipers.

    3. The plaster at the foot of an outside wall is bulging and has white salt patches. What does the technician do before the plaster is repaired?

      Check my answer
      See the worked solution

      The technician first finds and stops the water source, such as an overflowing gutter, a leaking pipe, splash-back from hard paving, or ground water, because the salts are carried to the surface by water. Plaster over a wet base will fail again, so the repair waits until the wall has dried.

    4. A diagonal crack from the top corner of a patient room window keeps getting longer, and the window has become hard to open. What does the technician do?

      Check my answer
      See the worked solution

      The technician does not patch the crack, marks its ends with the date, measures its width, photographs it, records the sticking window, and reports to the building manager to call a structural engineer. A lengthening diagonal crack from the corner of an opening together with a sticking window is a sign of a crack suspected to be structural and active.

    5. In a foil test on a basement storeroom wall, water forms on the outer surface of the foil, not behind it. What does that mean?

      Check my answer
      See the worked solution

      Water on the outer surface of the foil comes from humid air condensing on a cold surface, not from water passing through the wall. The response is directed at the humidity of the air and the ventilation of the room, as in Chapter 9 · Biology & Microbiology on mold.

    6. Why should a mason not use mortar harder than the bricks to fill a cracked joint in an old brick wall?

      Check my answer
      See the worked solution

      Mortar stronger than the bricks leaves no room for movement, so the stress from expansion, shrinkage, moisture, or settlement is released through the bricks and damages them permanently. A softer, more vapor-permeable mortar makes the damage happen in the joint, which is easier to repair.

    References

    External sources

    • Preservation Brief 15: Preservation of Historic Concretenps.gov
    • Preservation Brief 21: Repairing Historic Flat Plaster: Walls and Ceilingsnps.gov
    • Preservation Brief 39: Holding the Line: Controlling Unwanted Moisture in Historic Buildingsnps.gov
    • Preservation Brief 2: Repointing Mortar Joints in Historic Masonry Buildingsnps.gov
    • High Speed Two Phase One Information Paper C3: Ground Settlementassets.publishing.service.gov.uk

    Revision history

    DateVersionChange
    November 13, 20261First published

    How to cite

    Kurnia (2026). Cracks in walls and concrete: types and causes of cracks, structural and nonstructural cracks, measuring and monitoring crack width, seepage and dampness, plaster repair, and when to call a structural engineer. ARSTEMA Academy. Revised November 13, 2026. arstema.com/en/academy/konsep/retak-pada-dinding-dan-beton-jenis-dan-penyebab-retak-retak-struktural-dan-nonstruktural-mengukur-dan-memantau-lebar-retak-rembesan-dan-lembap-perbaikan-plester-serta-kapan-memanggil-ahli-struktur

    Self-check · 3 questions

    Check your understanding before moving on

    Write your answer in your own words, then compare it with the worked solution from this chapter’s exercises. The system doesn’t judge open answers as right or wrong; you decide which parts you’ve understood.

    0/3rated
    1

    A 30 m concrete wall without expansion joints undergoes a temperature change of 20 K. With α=10×10−6\alpha = 10 \times 10^{-6} per K, what is its free change in length, and what does it mean for cracks at its ends?

    2

    A plaster crack reads 0.20 mm in January and 0.22 mm in July on a gauge card with a resolution of 0.05 mm. Is the crack proven to be moving or proven to be still?

    3

    The plaster at the foot of an outside wall is bulging and has white salt patches. What does the technician do before the plaster is repaired?

    Self-assessment progress0%